CuZr0.1 is a zirconium-precipitation-strengthened copper alloy. With a conductivity of 90% IACS. Along with high-purity copper alloys, the alloy maintains almost the same value of conductivity; therefore, the strength increases. Apart from this, the CuZr0.1 alloy also exhibits better resistance to thermal than copper, better technological and relaxation properties than copper.
Information Of C15100
| Chemical composition(%) | Thickness (mm) | Grade
|
| GB | ASTM | EN | JIS |
| 0.08-3.0 |
| ≥99.8 | 0.05-0.15 | —— | TZr0.1 | C15100 | CuZr0.1 | C1510 |
|
| Physical properties |
Density (g/cm³) | Modulus of elasticity (GPa) | Thermal expansion coefficient (×10-6/K) | Electrical conductivity (%IACS) | Thermal conductivity W(m·K) |
| 8.9 | 121 | 17.6 | 90 | 350 |
| Mechanical properties | Bend properties |
| Temper | Hardness HV | Tension test | 90°R/T(Thick<0.8mm) |
Tensile Strength Rm/MPa | Yield Strength MPa | Elongation % | Good way | Bad way |
| H01 | 80-110 | 280-320 | ≥180 | ≥22 | 0 | 0 |
| H02 | 90-120 | 300-360 | ≥240 | ≥15 | 0.5 | 0.5 |
| H03 | 100-130 | 330-390 | ≥310 | ≥8 | 1 | 1 |
| H04 | 110-140 | 370-430 | ≥350 | ≥4 | 1.5 | 1.5 |
| H06 | 120-150 | 410-460 | ≥395 | ≥2 | 2 | 2 |
| H08 | ≥140 | 440-500 | ≥420 | ≥1 | 2.5 | 2.5 |